WEKO3
アイテム
TRIP鋼のねじり特性
https://nagano-nct.repo.nii.ac.jp/records/101
https://nagano-nct.repo.nii.ac.jp/records/1012b7b40a1-9a94-416c-82c7-07d8dd4a35e6
名前 / ファイル | ライセンス | アクション |
---|---|---|
KJ00004093390.pdf (814.6 kB)
|
Item type | Departmental Bulletin Paper(1) | |||||||
---|---|---|---|---|---|---|---|---|
公開日 | 2012-06-01 | |||||||
タイトル | ||||||||
タイトル | TRIP鋼のねじり特性 | |||||||
タイトル | ||||||||
タイトル | Mechanical Properties in Torsion of a TRIP Steel | |||||||
言語 | en | |||||||
言語 | ||||||||
言語 | jpn | |||||||
キーワード | ||||||||
主題Scheme | Other | |||||||
主題 | ねじり | |||||||
キーワード | ||||||||
主題Scheme | Other | |||||||
主題 | 残留オーステナイト | |||||||
キーワード | ||||||||
主題Scheme | Other | |||||||
主題 | 温間加工 | |||||||
キーワード | ||||||||
主題Scheme | Other | |||||||
主題 | せん断応力 | |||||||
キーワード | ||||||||
主題Scheme | Other | |||||||
主題 | ひずみ誘起変態 | |||||||
資源タイプ | ||||||||
資源タイプ識別子 | http://purl.org/coar/resource_type/c_6501 | |||||||
資源タイプ | departmental bulletin paper | |||||||
その他(別言語等)のタイトル | ||||||||
その他のタイトル | Mechanical Properties in Torsion of a TRIP Steel | |||||||
著者 |
長坂, 明彦
× 長坂, 明彦 |
|||||||
著者別名 |
NAGASAKA, Akihiko
× NAGASAKA, Akihiko
WEKO
0
|
|||||||
抄録 | ||||||||
内容記述タイプ | Abstract | |||||||
内容記述 | In the present work, to improve the workability of a 0.19C-1.54Si-1.52Mn (mass%) high-strength TRIP type multiphase (TMP) steel used warm forming, the effects of forming rate and forming temperature on mechanical properties in torsion were investigated. The TMP steel for a solid cylindrical specimen which was subjected to a torsional moment at one end was investigated at torsional strain rates between 0.002s^<-1> and 0.8 s^<-1>, and temperatures between 20℃ and 250℃. The shearing strain did not constantly depend on the torsional strain rate though the high strain rate of TMP steel decreased the maximum shearing stress, and raised the shearing yeild stress in the torsion characteristic at the room temperature. Furthermore, the torsional strain was increased by warm forming at about 150℃, at which the strain-induced transformation of retained austenite was suppressed most. | |||||||
書誌情報 |
長野工業高等専門学校紀要 en : Memoirs of Nagano National College of Technology 巻 38, p. 7-13, 発行日 2004-06-30 |
|||||||
出版者 | ||||||||
出版者 | 長野工業高等専門学校 | |||||||
ISSN | ||||||||
収録物識別子タイプ | ISSN | |||||||
収録物識別子 | 0286-1909 | |||||||
書誌レコードID | ||||||||
収録物識別子タイプ | NCID | |||||||
収録物識別子 | AN00179170 | |||||||
フォーマット | ||||||||
内容記述タイプ | Other | |||||||
内容記述 | application/pdf | |||||||
著者版フラグ | ||||||||
出版タイプ | VoR | |||||||
出版タイプResource | http://purl.org/coar/version/c_970fb48d4fbd8a85 |